产品详情
对应标准 ISO 9328-7-2018
不锈钢承压扁钢制品
Steel flat products for pressure purposes - Technical delivery conditions - Stainless steels
归类 奥氏体不锈钢
X2CrNiMoN18-12-4 化学元素成分含量(%)
成分 | C | Si | Mn | P | S | Cr | Ni | Mo | N |
最小值 | - | - | - | - | - | 16.5 | 10.5 | 3 | 0.1 |
最DA值 | 0.03 | 1 | 2 | 0.045 | 0.015 | 19.5 | 14 | 4 | 0.2 |
X2CrNiMoN18-12-4 机械性能 | ||||
厚度 | 抗拉强度 | 屈服点 | 延伸率 | 冲击吸收能量 |
t | σb | σs | δ | KV2 |
mm | Mpa | Mpa | % | J |
t≤8, 冷轧钢带 | 570~770 | ≥290 | ≥35 | ≥100 |
t≤13.5, 热轧钢带 | 570~770 | ≥270 | ≥35 | ≥100 |
t≤75, 热轧钢板 | 540~740 | ≥270 | ≥40 | ≥100 |